Plastics and Elastomers Notes FE Sem 2 Engineering Materials | MU
On this page
Plastics and rubbers are everywhere: water pipes, bottles, switch boards, non-stick pans, tyres, shoe soles, gaskets and medical tubing. Both are polymers, but plastics are moulded into rigid or semi-rigid shapes while elastomers stretch and spring back. This module introduces thermoplastic and thermosetting plastics, compounding of plastics and their applications, numericals on degree of polymerisation, density and mass, and tensile strength, then elastomers: the structural requirements of an elastomer, natural rubber, its processing, drawbacks and compounding. Finally it covers the preparation, properties and uses of two plastics, PMMA and PTFE, and two elastomers, polyurethane rubber and silicone rubber. It maps to course outcome CO4 and is the largest module of the course (5 hours).
Summary
Plastics: Plastics are high molecular mass organic polymers that can be shaped (moulded) by heat and pressure into articles that keep their shape at room temperature. They are light, corrosion resistant, good electrical and thermal insulators, easy to mould and colour, and cheap to mass produce, but they have lower strength and heat resistance than metals, can burn, and many do not biodegrade.
Thermoplastics and thermosetting plastics: Thermoplastics are made of linear or slightly branched chains held by weak van der Waals forces; they soften on heating and harden on cooling again and again, so they can be remoulded and recycled, and they dissolve in suitable solvents. Most are addition polymers: polyethylene, PVC, polystyrene, PMMA, PTFE, nylon (a condensation thermoplastic). Thermosetting plastics form a three-dimensional cross-linked network during moulding (curing); once set, they do not soften on reheating and cannot be remoulded, are insoluble, harder, stronger and more heat resistant, and are usually condensation polymers: Bakelite (phenol-formaldehyde), urea-formaldehyde, melamine-formaldehyde, epoxy resins.
Compounding of plastics: A pure polymer resin seldom has all the properties needed, so it is mixed with additives before moulding. Compounding ingredients: the resin or binder (main polymer, holds everything together); plasticisers (dibutyl phthalate, tricresyl phosphate, vegetable oils) that reduce intermolecular forces and make the plastic soft and flexible; fillers (wood flour, mica, china clay, glass fibres, carbon black, cotton flock) that reduce cost and improve hardness, strength, heat resistance or dimensional stability; dyes and pigments for colour; stabilisers (lead and barium salts, organotin compounds) that stop degradation by heat and light, especially in PVC; lubricants (waxes, oils, metal stearates) that make moulding easy and give a glossy finish; catalysts or accelerators (hydrogen peroxide, benzoyl peroxide, metal oxides, hexamine for phenolic resins) that speed up curing of thermosets; and antioxidants and flame retardants.
Applications of plastics: packaging (bottles, films, containers), building (pipes, window frames, flooring, insulation), electrical (wire insulation, switches, sockets, circuit boards), automobiles and aircraft (bumpers, dashboards, light covers), medical (syringes, blood bags, implants), household goods, textiles, sports goods and optical items.
Elastomers and their structural requirements: An elastomer is a polymer that can be stretched to several times its length under stress and returns rapidly to its original shape when the stress is removed. For this, the polymer must (i) have long, flexible, coiled chains; (ii) be amorphous in the unstretched state; (iii) have weak intermolecular forces; (iv) have a glass transition temperature well below the temperature of use; and (v) have a few cross-links between chains, which stop the chains slipping past each other permanently. Stretching straightens the coiled chains; when released they coil again, mainly because the coiled state has higher entropy.
Natural rubber: Natural rubber is cis-1,4-polyisoprene, a polymer of isoprene (2-methyl-1,3-butadiene, CH2=C(CH3)-CH=CH2). It is obtained from latex, a milky colloidal dispersion of rubber (about 30 to 40 percent) in water, which flows out when the bark of the rubber tree Hevea brasiliensis is cut (tapped). The all-cis structure gives coiled chains that cannot pack easily, so natural rubber is elastic. Gutta-percha, the trans isomer, is hard and not elastic.
Processing of natural rubber: Latex is collected and diluted to about 15 to 20 percent rubber, strained to remove dirt and bark, and coagulated by adding dilute acetic or formic acid. The soft coagulum is processed into (i) crepe rubber, by passing it through rollers to thin, crinkled sheets dried in air at about 40 to 50 °C, or (ii) smoked sheet rubber, by passing it through grooved rollers and drying the sheets in smoke houses at about 40 to 50 °C; the smoke acts as a preservative. Before compounding, raw rubber is masticated (worked between rollers) to break chains and make it soft and plastic.
Drawbacks of raw natural rubber: it becomes soft and sticky when hot and hard and brittle when cold, so it is useful only over a narrow range (roughly 10 to 60 °C); it has low tensile strength and poor abrasion resistance; on large stretching it suffers permanent deformation because chains slip; it absorbs water; it swells and dissolves in oils and organic solvents; and its double bonds are attacked by oxygen, ozone and oxidising agents, so it perishes (cracks) with age.
Compounding of rubber and vulcanisation: Raw rubber is mixed with: vulcanising agents (sulphur, or sulphur monochloride for cold curing; about 3 to 5 percent S gives soft rubber, about 30 to 50 percent gives hard rubber or ebonite); accelerators (mercaptobenzothiazole, tetramethylthiuram disulphide, zinc dithiocarbamates) that cut vulcanisation time and temperature; activators (zinc oxide with stearic acid); antioxidants (aromatic amines, phenols) against ageing; reinforcing fillers (carbon black, zinc oxide) that increase strength and wear resistance; inert fillers (whiting or CaCO3, clay, barytes) that reduce cost; softeners and plasticisers (vegetable oils, waxes, stearic acid); and colouring agents (titanium dioxide, iron oxide, lithopone). Vulcanisation is heating the compounded rubber with sulphur at about 100 to 140 °C; sulphur bridges form between chains at the double bonds. Vulcanised rubber has much higher tensile strength and elasticity, a wider useful temperature range, better resistance to abrasion, oils and solvents, and is not sticky.
Commercial polymers: PMMA (Perspex, Plexiglas) and PTFE (Teflon) are important plastics; polyurethane rubber and silicone rubber are important synthetic elastomers. Their preparation, properties and uses are tabulated below.
Numericals: Degree of polymerisation (DP) is the number of repeat units in a chain, DP = molecular mass of polymer / molecular mass of repeat unit. Density = mass/volume. Tensile strength = maximum load / original cross-sectional area, in N/mm² (= MPa).
Mind map
Plastics and Elastomers
- Plastics
- Thermoplastic: linear, remouldable
- Thermosetting: cross-linked, permanent set
- Compounding: resin, plasticiser, filler, stabiliser, lubricant, pigment, catalyst
- Applications
- Numericals
- DP = M / m0
- Density = m / V
- Tensile strength = F / A
- Elastomers
- Long coiled flexible chains
- Amorphous, low Tg, few cross-links
- Natural rubber: cis-polyisoprene
- Latex, coagulation, crepe and smoked sheet
- Drawbacks of raw rubber
- Compounding and vulcanisation
- Commercial polymers
- PMMA: transparent plastic
- PTFE: inert, non-stick
- Polyurethane rubber
- Silicone rubber
Thermoplastics versus thermosetting plastics
| Thermoplastics | Thermosetting plastics |
|---|---|
| Linear or slightly branched chains | Three-dimensional cross-linked network |
| Chains held by weak van der Waals forces | Chains joined by strong covalent cross-links |
| Soften on heating and harden on cooling repeatedly | Set permanently on heating; do not soften again |
| Can be remoulded and recycled | Cannot be remoulded or recycled easily |
| Soluble in some organic solvents | Insoluble in almost all solvents |
| Softer, weaker, less heat resistant | Harder, stronger, more brittle and heat resistant |
| Usually addition polymers | Usually condensation polymers |
| Polyethylene, PVC, polystyrene, PMMA, PTFE, nylon | Bakelite, urea-formaldehyde, melamine, epoxy resin |
Preparation, properties and uses of commercial polymers
| Polymer | Preparation | Properties | Uses |
|---|---|---|---|
| Polymethyl methacrylate (PMMA; Perspex, Plexiglas) | Free radical addition polymerisation of methyl methacrylate, CH2=C(CH3)COOCH3, using a peroxide initiator such as benzoyl peroxide (bulk or suspension) \( n\,\text{CH}_2{=}\text{C(CH}_3)\text{COOCH}_3 \rightarrow [\text{-CH}_2\text{-C(CH}_3)(\text{COOCH}_3)\text{-}]_n \) | Amorphous thermoplastic; highly transparent (about 92% light transmission, as clear as good glass); light (density about 1.18 g/cm³), about half as dense as glass; hard and rigid but scratches easily; good weather and UV resistance; softens near 100 to 110 °C; good electrical insulator; dissolves in acetone and chlorinated solvents | Aircraft and car windows, tail-light covers, lenses, signboards and displays, skylights, dentures and dental fillings, bone cement, intraocular and hard contact lenses, aquariums |
| Polytetrafluoroethylene (PTFE; Teflon) | Free radical polymerisation of tetrafluoroethylene, CF2=CF2, under pressure in water with a peroxide or persulphate initiator \( n\,\text{CF}_2{=}\text{CF}_2 \rightarrow [\text{-CF}_2\text{-CF}_2\text{-}]_n \) | Highly crystalline thermoplastic; melts at about 327 °C and is usable up to about 260 °C; density about 2.2 g/cm³; extremely inert, attacked only by molten alkali metals and fluorine at high temperature; very low coefficient of friction (non-stick); water repellent; excellent electrical insulator; cannot be processed by ordinary moulding, so it is shaped by sintering | Non-stick cookware coating, gaskets, seals, valve and pump packings, self-lubricating bearings, insulation of wires and cables, linings of chemical equipment, plumber's thread-seal tape, artificial blood vessels |
| Polyurethane rubber | Addition (step-growth) polymerisation of a diisocyanate with a diol or polyol, without any by-product \( n\,\text{OCN-R-NCO} + n\,\text{HO-R}'\text{-OH} \rightarrow [\text{-CO-NH-R-NH-CO-O-R}'\text{-O-}]_n \) Example: hexamethylene diisocyanate + ethylene glycol; toluene diisocyanate with polyester or polyether polyols | Excellent abrasion and tear resistance, high tensile strength and hardness range; resistant to oils, oxygen and ozone; flexible at low temperature; attacked by acids, alkalis and hot water (hydrolysis); foams form when water is added (CO2 released) | Foam mattresses, cushions and car seats, shoe soles, coatings and varnishes, gaskets, trolley and skate wheels, conveyor belts, elastic fibres (spandex), adhesives, thermal insulation |
| Silicone rubber (polydimethylsiloxane) | Hydrolysis of dimethyldichlorosilane to dimethylsilanediol, then condensation polymerisation; the long chains are cross-linked (cured) with a peroxide, usually with silica filler \( (\text{CH}_3)_2\text{SiCl}_2 + 2\text{H}_2\text{O} \rightarrow (\text{CH}_3)_2\text{Si(OH)}_2 + 2\text{HCl} \) \( n(\text{CH}_3)_2\text{Si(OH)}_2 \rightarrow [\text{-Si(CH}_3)_2\text{-O-}]_n + n\text{H}_2\text{O} \) | Si-O backbone: stays flexible from about -60 to over 200 °C; resistant to heat, oxidation, ozone, UV and weathering; water repellent; excellent electrical insulator; physiologically inert; lower tensile strength and tear resistance than other rubbers; swells in some hydrocarbon solvents | Gaskets, O-rings and seals for high and low temperature, cable insulation, sealants, medical implants, catheters and tubing, baby bottle nipples, bakeware, keypads, encapsulation of electronics |
Important definitions
| Term | Meaning |
|---|---|
| Plastic | A high polymer that can be moulded into a desired shape by heat and pressure. |
| Thermoplastic | A plastic that softens on heating and hardens on cooling repeatedly without chemical change. |
| Thermosetting plastic | A plastic that becomes permanently hard on heating due to cross-linking and cannot be remoulded. |
| Compounding | Mixing a polymer with additives such as plasticisers, fillers and stabilisers to obtain useful properties. |
| Plasticiser | An additive that reduces intermolecular forces and increases flexibility of a plastic. |
| Degree of polymerisation | The number of repeating units in a polymer chain. |
| Tensile strength | The maximum tensile stress a material can bear before breaking, load at break / original area. |
| Elastomer | A polymer that can be stretched greatly and returns quickly to its original shape when released. |
| Latex | A milky colloidal dispersion of rubber particles in water obtained from rubber trees. |
| Mastication | Mechanical working of raw rubber on rollers to break chains and make it soft and plastic. |
| Vulcanisation | Heating rubber with sulphur so that sulphur cross-links form between chains, improving its properties. |
| Glass transition temperature (Tg) | The temperature below which an amorphous polymer is hard and glassy and above which it is soft and rubbery. |
Formulas
| Formula | Meaning |
|---|---|
| \( \text{DP} = \dfrac{\bar M_{polymer}}{M_{repeat\ unit}} \) | Degree of polymerisation. |
| \( \bar M_n = \dfrac{\sum N_iM_i}{\sum N_i} \) | Number average molecular mass (Ni molecules of mass Mi). |
| \( \bar M_w = \dfrac{\sum N_iM_i^2}{\sum N_iM_i} \) | Weight average molecular mass; PDI = Mw/Mn. |
| \( \rho = \dfrac{m}{V},\ m = \rho V \) | Density and mass of a polymer article. |
| \( \sigma_{TS} = \dfrac{F_{max}}{A_0} \) | Tensile strength (N/mm² = MPa); for a rod \(A_0 = \pi d^2/4\). |
Repeat unit masses: ethylene C2H4 28.05; vinyl chloride C2H3Cl 62.50; styrene C8H8 104.15; methyl methacrylate C5H8O2 100.12; tetrafluoroethylene C2F4 100.01 g/mol.
Key points to remember
- Thermoplastics: linear, remouldable, recyclable. Thermosets: cross-linked, permanent set.
- Plasticisers give flexibility; fillers reduce cost and add strength; stabilisers protect against heat and light.
- Elastomer needs long coiled chains, amorphous structure, low Tg and a few cross-links.
- Natural rubber = cis-1,4-polyisoprene; gutta-percha = trans form, not elastic.
- Latex is coagulated with acetic or formic acid; crepe and smoked sheet are the two forms.
- Raw rubber: sticky when hot, brittle when cold, weak, attacked by oxygen and solvents.
- Vulcanisation: 3 to 5% S gives soft rubber; 30 to 50% S gives ebonite.
- PMMA: transparent, light, weather resistant. PTFE: most chemically inert, non-stick, m.p. about 327 °C.
- Polyurethane: diisocyanate + diol, no by-product. Silicone rubber: Si-O backbone, wide temperature range.
Solved examples
Example 1. A PMMA sample has an average molecular mass of 150000 g/mol. Find its degree of polymerisation.
Repeat unit C5H8O2 = 5(12.01) + 8(1.008) + 2(16.00) = 100.12 g/mol. DP = 150000/100.12 = 1498, about 1500.
Example 2. Find the DP of polyethylene of molecular mass 28000 g/mol, and the molecular mass of PTFE with DP 5000.
PE: DP = 28000/28.05 = 998, about 1000. PTFE: M = 5000 x 100.01 = 5.0 x 105 g/mol.
Example 3. A polymer sample has 100 molecules of mass 10000 and 200 molecules of mass 20000. Find Mn, Mw and the polydispersity index.
\( \bar M_n = (100\times10^4 + 200\times2\times10^4)/300 = 5\times10^6/300 = 16667 \). \( \bar M_w = (100\times10^8 + 200\times4\times10^8)/(5\times10^6) = 9\times10^{10}/5\times10^6 = 18000 \). PDI = 18000/16667 = 1.08.
Example 4. A PTFE block 20 cm x 10 cm x 0.5 cm weighs 220 g. Find its density.
V = 20 x 10 x 0.5 = 100 cm³. Density = 220/100 = 2.2 g/cm³, which matches PTFE.
Example 5. Find the mass of a PMMA sheet 1 m x 0.5 m x 5 mm (density 1.18 g/cm³).
V = 100 cm x 50 cm x 0.5 cm = 2500 cm³. Mass = 1.18 x 2500 = 2950 g = 2.95 kg.
Example 6. A PMMA rod of 10 mm diameter breaks under a tensile load of 5.5 kN. Find its tensile strength.
\( A = \pi d^2/4 = \pi(10)^2/4 = 78.54 \) mm². Tensile strength = 5500/78.54 = 70.0 N/mm² = 70 MPa.
Example 7. A polyethylene strip 20 mm wide and 4 mm thick breaks at 2.4 kN. Find its tensile strength.
A = 20 x 4 = 80 mm². Tensile strength = 2400/80 = 30 N/mm² = 30 MPa.
Example 8. A PVC chain has DP 1200. Find its molecular mass.
M = 1200 x 62.50 = 75000 g/mol.
Important questions and answers
Q1. Distinguish between thermoplastics and thermosetting plastics. (4 marks)
Thermoplastics have linear or slightly branched chains held by weak forces, soften on heating and harden on cooling repeatedly, can be remoulded and recycled, are soluble in some solvents, are softer and are mostly addition polymers (PE, PVC, PS, PMMA). Thermosetting plastics have a cross-linked three-dimensional network, set permanently on heating, cannot be remoulded, are insoluble, harder, stronger and more heat resistant, and are mostly condensation polymers (Bakelite, urea-formaldehyde, epoxy).
Q2. What is compounding of plastics? Explain the role of any four ingredients. (5 marks)
Compounding is mixing a resin with additives to obtain a mouldable material with the desired properties. Resin (binder): the main polymer that binds the other ingredients. Plasticisers (dibutyl phthalate, tricresyl phosphate): reduce intermolecular forces, increase flexibility and reduce brittleness. Fillers (wood flour, mica, china clay, glass fibre): reduce cost, increase hardness, strength and heat resistance, reduce shrinkage. Stabilisers (lead and barium salts, organotin compounds): prevent degradation by heat and light, important for PVC. Lubricants (waxes, metal stearates): make moulding easy, prevent sticking to the mould, give glossy finish. Pigments and dyes: give colour. Catalysts or accelerators: speed up curing of thermosetting resins.
Q3. What are the structural requirements of an elastomer? (3 marks)
Long, flexible, randomly coiled chains; amorphous in the unstretched state; weak intermolecular forces; glass transition temperature well below room temperature; a small number of cross-links to prevent permanent slippage of chains; presence of double bonds or reactive sites that allow vulcanisation (cross-linking).
Q4. How is natural rubber obtained from latex? (4 marks)
The bark of Hevea brasiliensis is cut (tapped) and latex, about 30 to 40 percent rubber in water, is collected. It is diluted to about 15 to 20 percent, strained to remove dirt, and coagulated with dilute acetic or formic acid. The coagulum is made into crepe rubber (passed through rollers to thin crinkled sheets and air dried at 40 to 50 °C) or smoked sheet rubber (rolled with grooved rollers and dried in smoke houses at 40 to 50 °C). Before use it is masticated and compounded.
Q5. State the drawbacks of natural rubber and explain how vulcanisation removes them. (5 marks)
Drawbacks: soft and sticky when hot, brittle when cold (useful only about 10 to 60 °C); low tensile strength; permanent set on stretching; poor abrasion resistance; absorbs water; swells in oils and solvents; oxidised by air and ozone and perishes. Vulcanisation: compounded rubber is heated with sulphur (with accelerators and ZnO) at about 100 to 140 °C. Sulphur bridges form between neighbouring chains at the double bonds, converting the chains into a lightly cross-linked network. Result: tensile strength rises roughly ten times, elasticity becomes reversible, useful range becomes about -40 to 100 °C, resistance to abrasion, solvents and oxidation improves and stickiness disappears. Increasing sulphur gives harder rubber; 30 to 50 percent gives ebonite.
Q6. Explain compounding of rubber. (5 marks)
Vulcanising agent (sulphur, sulphur monochloride): forms cross-links. Accelerators (mercaptobenzothiazole, thiuram disulphides): reduce vulcanisation time and temperature. Activators (ZnO, stearic acid): increase accelerator efficiency. Antioxidants (aromatic amines, phenols): retard ageing by oxygen and ozone. Reinforcing fillers (carbon black, ZnO): increase tensile strength, stiffness and abrasion resistance; carbon black is used in tyres. Inert fillers (CaCO3, clay, barytes): reduce cost. Softeners and plasticisers (vegetable oils, waxes): make mixing easier and improve tenacity. Colouring agents (TiO2, iron oxide, lithopone).
Q7. Give the preparation, properties and uses of PMMA and PTFE. (6 marks)
PMMA: free radical polymerisation of methyl methacrylate with benzoyl peroxide; transparent, light (1.18 g/cm³), weather resistant, rigid, softens near 100 °C, scratches easily; used for aircraft and car windows, lenses, signboards, dentures, bone cement. PTFE: free radical polymerisation of tetrafluoroethylene under pressure with a peroxide or persulphate initiator in water; highly crystalline, melts at about 327 °C, extremely inert, very low friction, excellent insulator, water repellent; used for non-stick coatings, gaskets, seals, bearings, cable insulation, chemical plant linings. Equations as in the table above.
Q8. Give the preparation, properties and uses of polyurethane rubber and silicone rubber. (6 marks)
Polyurethane: a diisocyanate (for example hexamethylene diisocyanate) reacts with a diol (ethylene glycol) or polyol by addition without by-product, forming urethane (-NH-CO-O-) links; tough, abrasion and tear resistant, resistant to oil and ozone, attacked by acids and alkalis; used for foams, shoe soles, coatings, wheels, spandex fibres, adhesives. Silicone rubber: (CH3)2SiCl2 is hydrolysed to (CH3)2Si(OH)2, which condenses to polydimethylsiloxane, then cross-linked with peroxide; flexible from about -60 to over 200 °C, resistant to heat, oxidation and weathering, water repellent, insulating and biologically inert, but of low tensile strength; used for gaskets and seals, cable insulation, sealants, medical implants and tubing, bakeware.
Q9. Find the DP of polystyrene of molecular mass 2.08 x 105 g/mol. (2 marks)
Repeat unit C8H8 = 104.15. DP = 208000/104.15 = 1997, about 2000.
Exam tips
- Write the monomer, the polymerisation equation, three properties and three uses for each of PMMA, PTFE, polyurethane and silicone rubber.
- Draw the repeat unit correctly inside square brackets with n outside.
- For differences, use a two-column table with at least six points.
- In tensile strength numericals convert kN to N and use mm² so the answer comes in MPa.
- Show the molar mass of the repeat unit step by step in DP questions.
- Mention the role of each compounding ingredient with one example chemical.
FAQs
Why is PTFE so unreactive?
Its carbon chain is completely covered by fluorine atoms, and the C-F bond is one of the strongest single bonds. Nothing can easily reach or break the backbone.
Why does vulcanised rubber return to shape while raw rubber does not?
In raw rubber the stretched chains slide past each other and stay displaced. Sulphur cross-links tie the chains together, so they can uncoil but not slip, and they recoil when released.
Why is silicone rubber used in ovens and space applications?
Its Si-O backbone is much more stable to heat and oxidation than a C-C backbone. It stays rubbery over a very wide temperature range.
Is nylon a thermoplastic even though it is a condensation polymer?
Yes. Its chains are linear and not cross-linked, so it softens on heating and can be remoulded.
These notes follow the University of Mumbai first-year engineering syllabus (NEP 2020, Engineering Materials) and were prepared with AI help and checked.
More in Engineering Materials
See all →- Alloys Notes FE Sem 2 Engineering Materials | MU MU FE Engineering Materials Module 1: carbon, heat, shock and stainless steels, alloying elements, duralumin, brass, bronze, Wood's metal, n...
- Ceramics Notes FE Sem 2 Engineering Materials | MU MU FE Engineering Materials Module 2: ceramics types, properties and uses, glass and its types, natural and artificial abrasives, optical fi...
- Composites Notes FE Sem 2 Engineering Materials | MU MU FE Engineering Materials Module 3: matrix and reinforcement, fibre-reinforced, laminated and particulate composites, bio-composites and t...
- Advanced Polymers Notes FE Sem 2 Engineering Materials | MU MU FE Engineering Materials Module 5: conducting polymers and doping, biopolymers, liquid crystal polymers and smart polymers with applicati...
- Nano Materials Notes FE Sem 2 Engineering Materials | MU MU FE Engineering Materials Module 6: nanomaterials and their types (0D to 3D), applications, graphene, and SWCNT vs MWCNT properties and us...